Products

T8 DIP Tube Light

The material performance of piezoelectric ceramic

The material performance of piezoelectric ceramic

 

The material performance of piezoelectric ceramic
Num
Name of Performance parameter
symbol
index
Allow the public errand
P-33
 
P-43
P-44
P-51
P-52
 
 
P-81
1
Electromechanical coupling coefficient
Kp
0.60
 
0.58
0.60
0.65
0.64
 
 
0.53
±6.0%
K31
0.36
 
0.34
0.36
0.38
0.37
 
 
0.31
K33
0.70
 
0.67
0.70
0.74
0.76
 
 
0.63
K15
0.70
 
0.67
0.70
0.72
0.75
 
 
0.66
Kt
0.47
 
0.48
0.48
0.50
0.49
 
 
0.47
2
The relative electric capacity rate of freedom
ε
T
1725
 
1275
1350
2100
3250
 
 
1025
±12.5%
ε
T
1725
 
1700
1900
2400
3500
 
 
1400
3
The medium losses
tgδ
0.020
0.006
0.005
0.020
0.020
 
 
0.004
4
The gentle and agreeable constant of elasticity
(x10-12m2/N)
S
E
11
15
 
11.5
13
15
15.5
 
 
11.0
±10%
S
D
33
9.0
 
8.0
8.5
9.0
9.0
 
 
8.5
S
D
55
25
 
21.0
21.5
22.0
23.0
 
 
21.0
5
Piezoelectricity meet an emergency the constant
(x10-12m/v或C/N)
d31
160
 
-130
-150
-210
-260
 
 
-100
±12.5%
d33
390
 
290
320
450
575
 
 
225
d15
480
 
500
530
710
950
 
 
450
6
Mechanical cue
Qm
75
 
500
400
70
65
 
 
800
7
Frequency constant
(Hz•m)
Nd
1950
2200
2200
2000
1940
 
 
2300
±5%
N1
1470
 
1700
1600
1450
1450
 
 
1700
N3
1880
 
2050
2000
1900
1900
 
 
1960
N5
1130
 
1230
1230
1200
1200
 
 
1230
Nt
2250
 
2300
2300
2250
2300
 
 
2280
8
The velocity of sound
(m/s)
Vd
3000
 
3500
3300
3000
3010
 
 
3500
±5%
V1
2940
 
3400
3200
2900
2900
 
 
3400
V3
3760
 
4100
4000
3800
3800
 
 
3920
V5
2260
 
2460
2460
2400
2400
 
 
2460
Vt
4500
 
4600
4600
4500
4600
 
 
4560
9
Density (x103kg/m3)
ρ
7.6
 
7.45
7.5
7.45
7.4
 
 
7.45
10
Curie´s temperature (℃)
Tc
335
 
300
300
260
180
 
 
300
11
Rate of change of time of ten times
(%)
ANd
0.20
 
1.3
1.2
0.35
0.35
 
 
1.3
 
AKp
-0.25
 
-2.0
-1.8
-0.4
-0.25
 
 
-2.0
-1.5
 
-4.5
-4.0
-1.5
-2.0
 
 
-4.0
12
The relative rate of change of temperature (%)-10℃~50℃ The datum 25℃
ΔNd/N
1.0
 
1.5
1.0
1.5
2.0
 
 
1.5
 
Δε/ε
15
 
9.5
9.0
20
40
 
 
9.0
 
13
The strong field lies between electric performance
T=25℃ E=400V
tgδ
 
 
0.04
0.04
 
 
 
 
0.01
Δε/ε
 
 
0.20
0.17
 
 
 
 
0.06
note: 1, Index besides Curie´s temperature, is the measurement value for ten days after polarizing for the performance parameter index in the form .

 